Polyetherketoneketone (PEKK)

Note

PEKK and its filled carbon fiber version are classified as experimental materials for advanced users.

Info

While you are free to use any brand and type of material you wish on your AON3D machine, we can only provide support for AON3D-approved materials that we have tested and developed processes for in-house, all of which can be purchased from AON3D directly by contacting sales@aon3d.com.

General Process Settings

Setting Value
Extrusion Temperature 320-360ºC
Bed Temperature 120-160ºC
Chamber Temperatures 110ºC

Usage Notes

Build Surface Preparation

PEKK prints best on the High Temperature PEI build plate with the use of a brim or raft. Note that surface of the PEI plate should be periodically resurfaced using a mill, or with an orbital palm sander if no milling services are available. Please contact sales@aon3d.com if you currently have a PEI film surfaced aluminum build plate and would like to upgrade to a High Temperature PEI Build Plate surfaced aluminum build plate.

Material Pre-treatment

PEKK is susceptible to moisture uptake. We recommend drying the filament overnight at 100ºC before use, and to always store in a sealed container with dessicant. Take care to check the spool material of your filament prior to baking your material. Some vendors use low temperature materials for spools which may melt or deform at bakeout temperature.

Please contact help@aon3d.com for any questions on this matter.

Support Material

There is currently no compatible support material for PEKK - prints will require self-support.


Sample Slicer Profiles

Assumes 0.6mm nozzle installed.

PEKK: Single Extruder

CF-PEKK: Single Extruder